江西某地白钨矿浮选试验研究
- 格式:pdf
- 大小:227.21 KB
- 文档页数:4
江西某硫尾矿中白钨矿的浮选回收试验罗文;邵辉【摘要】江西某硫尾矿中有用矿物主要为白钨矿,WO3含量为0.22%。
为确定该尾矿中白钨矿的回收工艺,在实验室进行了选矿试验。
结果表明:试样采用1粗3精3扫常温浮选,常温精矿以水玻璃为脱药剂在90℃下搅拌脱药,再采用1粗4精3扫加温浮选流程处理,最终得到WO3品位为67.03%、回收率为76.17%的白钨精矿。
%The sulfur tailings from Jiangxi contain 0.22% WO3 .For determining the recovery process of scheelite from tailings,the mineral processing experiments were investigated in lab.The results show the scheelite concentrate with WO3 grade of 67.03% and recovery of 76.17% can be got by adopting the normal temperature flotation of single-stage roughing,three-stage cleaning,three-stage scavenging,sodium silicate as reagent removal agent,stirring at 90 ℃,then the heating flotation of cleaning flowsheet of single-stage roughing,four-stage cleaning and three-stage scavenging process.【期刊名称】《金属矿山》【年(卷),期】2016(000)007【总页数】3页(P186-188)【关键词】硫尾矿;白钨矿;常温浮选;加温浮选【作者】罗文;邵辉【作者单位】武汉理工大学资源与环境工程学院,湖北武汉430070;武汉理工大学资源与环境工程学院,湖北武汉430070【正文语种】中文【中图分类】TD923+.7钨是一种应用广泛的稀有金属。
难选低品位白钨矿选矿试验研究1前言江西某多金属矿山矿产资源丰富,除铁矿石外,还共生有白钨、铅、锌、铜等多种有色金属,探明铁矿石表内储量600多万吨,表外储量500多万吨,尤其是白钨,查明WO3储量1.66万吨,其平均品位达0.155%左右。
到目前为止,仅对铁矿石进行了选矿回收,白钨等矿石作为选铁尾矿未作回收。
为保护国家矿产资源,提高资源利用率,节能减排,保护环境,提高矿山经济效益,矿方决定对矿山尾矿中的白钨开展回收工作。
本试验是受矿山的委托而进行的,其目的是对矿山尾矿中的白钨进行可选性试验研究,评价其可选性,提出回收白钨的工艺流程。
试验中进行了重选法、浮选法、重浮联合工艺等多个方案的比较试验。
试验表明,较好的分选方案为离心机作粗选浮选精选的重浮联合流程。
经离心机转速,浮选药剂种类用量等多个条件试验后,进行了闭路试验。
试验研究后,推荐的工艺流程如图1-1所示。
在图1-1的流程条件下,取得了较为理想的选别指标,可获得WO3为50.16%,回收率为70.22%的白钨精矿,实现了对白钨的分选回收。
2 矿石性质矿石中金属矿物主要为白钨矿、赤铁矿、褐铁矿和磁铁矿,含有少量闪锌矿、黄铜矿、方铅矿。
非金属矿物主要有透辉石、透闪石、石榴子石、粒硅美石、萤石及滑石等。
矿石中的铁主要含在赤铁矿、褐铁矿和磁铁矿中,少量含于含铁硅酸盐矿物和硫化物中。
白钨矿多图1-1 推荐的工艺流程图产于透辉石粒间和萤石、滑石脉中,少数与磁铁矿共生。
矿石的结构主要有交代结构,半自形—自形晶结构。
矿石的构造主要有条带状构造,柔皱构造和浸染状构造。
试样的多元素分析结果以及钨的物相分析结果分别见表2-1和表2-2。
表2-1试样多元素分析结果元素Fe WO3SiO2CaO MgO Al2O3含量/% 15.27 0.30 46.65 2.44 0.78 12.46 元素S Au含量/% 0.05 0.13注:金的含量单位为g/t。
表2-2试样钨的物相分析结果名称钨华黑钨白钨总钨含量/% 0.006 0.014 0.296 0.3163 脱泥与不脱泥方案确定对试样采用沉降水析法分别做了脱除–0.038mm以及–0.020mm粒级矿泥的试验。
某白钨矿伴生多金属硫化矿选矿试验研究
《某白钨矿伴生多金属硫化矿选矿试验研究》
一、研究背景
1、某白钨矿伴生多金属硫化矿,是一种常见的硫化矿,其开采难度较大。
主要因其中所含白钨矿具有比较高的品位,所以,加工利用这类硫化矿自然就成了一类重要选矿试验研究的内容。
同时,某白钨矿伴生多金属的分布也是本次研究的重点。
2、由于某白钨矿伴生多金属硫化矿是以层状分布的,从而影响了选矿工艺,
因此研究表明,应十分仔细地分析其伴生金属与白钨矿的层状分布特征,从而为后续的矿物加工提供参考依据。
二、施工和研究内容
1、开垦前某白钨矿伴生多金属硫化矿的矿脉特征:主要采回一定数量的样品,对某白钨矿伴生多金属硫化矿矿脉的形态、尺寸及其类型做出合理判断。
2、矿物加工选矿工艺:根据前期研究结果,确定矿物分布情况并制定适合当
地成矿区划分的矿物加工选矿工艺,以取得满足要求的结果。
3、研究结果分析:利用各种测试和分析技术,对本次研究所采取的矿物加工
选矿工艺进行定量分析,并得出结论。
三、结论
1、A某白钨矿伴生多金属硫化矿矿脉结构具有特殊的层状分布特征,这对选
择适宜的磨矿工艺有一定的影响,故应着重研究。
2、该研究结果显示,矿物加工选矿工艺能够明显提高A某白钨矿伴生多金属
硫化矿的精矿品位,从而满足相应的市场需求。
四、后续建议
1、在后续的研究中,应开展深入的矿物加工技术研究,以期望获得更优异的
结果。
2、在研究中,还可以引入其他相关内容,例如环境保护、资源效益等问题,认真探讨、进行改进和加强。
某白钨尾矿中伴生萤石的选矿试验丁军;黄超军;李少平;何桂春【摘要】江西某白钨浮选尾矿萤石、方解石含量均较高,CaF2、CaCO3含量分别为12.33%和9.79%,属于复杂难选伴生萤石二次资源.为从该二次资源中高效回收萤石,进行了详细的选矿试验.结果表明,酸性水玻璃+腐植酸钠组合使用可在浮选萤石时有效抑制方解石等脉石矿物.在氧化石蜡皂731总用量为1150 g/t,酸性水玻璃+腐植酸钠总用量为(2750+275)g/t的条件下,采用1次粗选、粗精矿再磨后6次精选、粗选尾矿和精选1尾矿各2次扫选流程处理试样,最终获得CaF2品位95.26%、回收率85.37%的萤石精矿,较好地实现了从白钨尾矿中综合回收萤石的目标.%The contents of fluorite and calcite in a Scheelite flotation tailing in Jiangxi are high with contents of CaF2and CaCO312.33% and 9.79% respectively.It belongs to a complex refractory secondary ore with fluorite contained.In order to efficiently recover fluorite from the secondary resources,a detailed beneficiation experiment was carried out.The results showed that the combination of acidic water glass and sodium humate effectively inhibited calcite and other gangue minerals in floata-tion of fluorite.Under addition of 731 oxidized paraffinum sodium salt 1 150g/t,the total dosage of acidic water glass+sodium humate (2 750+275)g/t,and by the process of one roughing,six cleanings of coarse concentrate after regrinding,two scaveng-ings for coarse tailings and tailings of cleaning one separately,fluorite concentrate with CaF2grade of 95.26% and the recovery rate of 85.37% was finally achieved,and targets at thecomprehensive recovery of fluorite from scheelite tailings were well real-ized.【期刊名称】《金属矿山》【年(卷),期】2018(000)003【总页数】5页(P187-191)【关键词】白钨矿浮选尾矿;萤石;酸性水玻璃+腐植酸钠组合抑制剂【作者】丁军;黄超军;李少平;何桂春【作者单位】江西理工大学资源与环境工程学院,江西赣州341000;江西省矿业工程重点实验室,江西赣州341000;江西理工大学资源与环境工程学院,江西赣州341000;江西省矿业工程重点实验室,江西赣州341000;江西理工大学资源与环境工程学院,江西赣州341000;江西省矿业工程重点实验室,江西赣州341000;江西理工大学资源与环境工程学院,江西赣州341000;江西省矿业工程重点实验室,江西赣州341000【正文语种】中文【中图分类】TD923+.7近20年来,我国经济的快速发展不断加速自然资源供应紧张的局面,贫、细、杂资源以及二次资源的开发利用就成为矿业界研究的课题[1]。
ZL捕收剂浮选白钨矿的研究和应用目前,我国白钨矿的回收方法主要是浮选,所使用的捕收剂主要是731氧化石蜡皂。
白钨矿的可浮性较好,但因矿石中存在与其性质相类似的含钙矿物如方解石、萤石和磷灰石等而导致浮游过程复杂化。
白钨矿与含钙矿物的浮选分离是影响白钨矿选别指标的重要因素,因此研制新捕收剂要尽量加大白钨矿与含钙脉石矿物可浮选性的差异.我们研制的ZL捕收剂是一种长碳羟酸皂化物的混合物,对白钨矿具有较强的选择捕收能力,对多种白钨矿矿石进行选矿试验,均获得了令人满意的结果.ZL捕收剂兼有起泡性、毒性低、无刺激性气味及性能稳定(可存放6个月以上),其合成原料易得,价格合适,目前,ZL捕收剂已经应用于一些中小型矿山的白钨矿浮选.1 ZL选别湖南某白钨矿矿石1.1矿石性质湖南临武某白钨矿矿床,主要金属矿物有白钨矿、黑钨矿和方铅矿等。
钨矿物以白钨矿为主,黑钨矿极少;主要脉石矿物有萤石、方解石、长石、石英、石榴石、绿泥石和磷灰石等。
原矿的主要成分(质量分数,)为:WO。
0.6,Pb 0.2O,Cu 0.008,Zn 0.01,CaFz 2O.56,CaCO3 13.9O,SiO2 41.5,Al2O。
7.21,CaO 3.47.原矿中白钨矿嵌布粒度范围较宽,粗至0.8ram,细至0.009mm,大多为0.O4~O.4mm,属于中细粒嵌布.当矿石的磨矿细度为8O 一0.074mm时,白钨矿单体解离率超过90%。
1.2小型试验由原矿性质可知,该矿石中含钙矿物的种类多、含量高,是较典型的难选白钨矿.在小型试验的粗选段分别以ZL和731氧化石蜡皂为捕收剂进行对比试验,试验流程如图1所示,试验结果列于表1.表1是两种捕收剂在较佳的用量范围内的对比试验结果.由表1可知,在捕收剂用量相同条件下,用ZL捕收剂获得的钨粗精矿品位和回收率都高于用731氧化石蜡皂.当731捕收剂用量增加时,钨回收率提高,但精矿品位下降较多,浮选泡沫量大且粘,上浮物夹杂脉石严重,这将给后面的粗精矿精选带来不良影响.使用ZL捕收剂浮选的泡沫量不大且较稳定,尾矿钨品位比用731氧化石蜡皂低.1.3工业试验在小型试验的基础上,该选矿厂分别用ZL与731进行了选钨的工业试验.试验的粗选段为两次精选、三次扫选,捕收剂用量为580 g/t,调整剂为1.2 kg/t NazC0。