某铅锌银多金属硫化矿选矿工艺研究王李鹏,任琳珠(西北矿冶研究院矿物工程研究所甘肃省白银市730900)摘要:针对某铅锌银多金属硫化矿矿石性质特点,综合考虑经济效益因素,提出采用铅部分优先-铅锌混合浮选工艺流程,配合采用选择性好的新型铅矿物捕收剂D25和新型锌矿物抑制剂T8,较好的实现了该矿石的综合回收。
实验室小型闭路试验获得铅精矿铅、银品位分别为70.30%、5886.55 g/t,回收率分别为48.27%、30.65%;铅锌混合精矿铅、锌、银品位分别为15.24%、45.06%、2846.36g/t,回收率分别为46.38%、93.25%、65.67%,铅、银总回收率94.65%、96.32%的较好指标。
关键词:多金属矿;部分优先浮选;混合浮选;银回收中图分类号:TD952 文献标识码:AExperimental Study on Beneficiation Process of a Lead-Zinc-SilverPolymetallic OreWang Li-peng REN Lin-zhu(Mineral Engineering Research Institute of Northwest Research Institute of Mining andMetallurgy,Baiyin,Gansu 730900)Abstract:According to the lead-zinc-silver polymetallic ore characteristics and in the view of economic benefit, the experiment developed lead partially preferential flotation and lead-zinc bulk flotation flowsheet adding the new type lead collector D25 and the new type zinc depressant T8.It can get the comprehensive recovery of the ore.Good indexes are obtained with lead concentrate containing 70.30% lead and 5886.55g/t silver, lead recovery of 48.27% and silver recovery of 30.65%;lead-zinc concentrate containing 15.24% lead ,45.06% zinc and 2846.36g/t silver, lead recovery of 46.38% ,zinc recovery of 93.25% and silver recovery of 65.67%;the total lead recovery of 94.65%and silver recovery of 96.32%.Keywords:polymetallic ore;partially preferential flotation;bulk flotation;silver recovery.铅锌矿作为重要的有色金属矿产资源,在国民经济发展中具有重要地位,广泛应用于各种行业和领域。
探析某银铅锌多金属硫化矿石选矿工艺发布时间:2021-07-02T14:18:02.130Z 来源:《中国科技信息》2021年8月作者:冉臣[导读] 文中结合某铅锌银多金属硫化矿对其选矿工艺进行分析研究,该矿矿石当中的铅以方铅矿的形式存在,锌存在形式主要为闪锌矿,银以辉银矿、银黝铜矿和深红银矿等形式存在新疆哈巴河阿舍勒铜业股份有限公司冉臣 836700摘要:文中结合某铅锌银多金属硫化矿对其选矿工艺进行分析研究,该矿矿石当中的铅以方铅矿的形式存在,锌存在形式主要为闪锌矿,银以辉银矿、银黝铜矿和深红银矿等形式存在,伴生方铅矿,为了对这些矿产资源进行科学的开发与利用,对该矿矿石选矿工艺进行深入探讨,通过研究发现,磨矿细度以-0.074mm占78%和石灰形成的PH值=11的碱性条件之下,铅银矿物捕收剂运用乙硫氮联合丁铵黑药、锌矿物抑制剂运用ZnSO4+Na2SO4,对浮选铅于伴生的银矿物进行优选,硫化铜作为浮铅银尾矿活化剂,而浮选铅锌矿捕收剂运用丁黄药,能够获得铅品位为57.05%、铅回收率为88.11%的铅精矿和锌品位为48.31%、锌回收率为86.29%的锌精矿,在铅锌金矿当中银达到87.99%的总回收率。
关键词:铅锌银硫化矿石;选矿工艺某银铅锌多金属硫化矿,属于热液充填型矿床,含有大量的多金属元素,矿床为中大型规模大小,矿石当中的有用组分较多,闪锌矿、方铅矿与半生的银矿物是该矿矿石当中的主要金属矿物,而且这些矿物成分具有非常复杂的共生关系,增加了矿石的选矿难度,导致长时间以来没有得到有效的开发利用。
为了对这些矿产资源进行有效的开发和利用,该文当中结合该银铅锌多金属硫化矿,通过试验研究分析其合适的选矿工艺,目标是在将铅、锌精矿分选出的同时,确保银矿物的高效回收,进而确保这些矿产资源,进而为这些矿产资源更加开发利用奠定坚实的基础。
1矿石性质矿石中铅、锌矿物主要赋存在方铅矿和闪锌矿中,银矿物主要以银黝铜矿、辉银矿、深红银矿等伴生银的形式存在;其他金属矿物为黄铜矿、黄铁矿、磁黄铁矿、白铅矿、白铁矿、铅矾、褐铁矿、毒砂等;非金属矿物有石英、绿泥石、角闪石、方解石、黑云母、绢云母、白云母、电气石、透闪石和炭泥质粉砂岩等。
某铜铅锌复杂多金属矿选矿试验研究第一章:引言1.1 研究背景及意义1.2 国内外研究现状分析1.3 研究目的及研究内容第二章:矿石性质及选矿工艺流程2.1 矿石物理性质2.2 矿石化学成分分析2.3 矿物学研究2.4 选矿流程选择第三章:试验方法及实验设计3.1 试验方法3.2 实验设计步骤3.3 实验条件及仪器设备介绍第四章:实验结果及分析4.1 磨矿实验结果4.2 分选实验结果4.3 浮选实验结果4.4 试剂对浮选的影响第五章:选矿实验结论及展望5.1 实验结论5.2 选矿工艺流程优化的趋势及展望参考文献第一章:引言1.1 研究背景及意义复杂多金属矿是指铜、铅、锌、金、银等多种贵重金属矿物在同一矿石中存在的矿石,其矿石经济价值极高。
然而,这些金属在矿石中的含量往往相对较低而且难以分离,因此矿石的选矿工艺变得尤为重要。
在矿石矿种复杂、矿物组成多样的铜铅锌复杂多金属矿中,研究如何实现有效地分离这些金属是一个十分复杂的课题,具有非常重要的意义。
由于铜铅锌复杂多金属矿的特殊性质,目前国内外对于该类矿物资源选矿技术的研究、应用与开发尚处于初步阶段。
因此,对该类矿物资源选矿技术的研究具有重要的现实意义和广泛的应用前景。
1.2 国内外研究现状分析国内外对于铜铅锌复杂多金属矿的选矿技术研究已有一定程度的深入,但始终无法得到广泛应用和局部发展。
国外研制和生产该类选矿技术的公司比较多,如加拿大Fluor公司和美国Fred Wells Engineering公司等。
国内以中冶试验研究院、中冶长沙研究院、中冶集团长沙冶金设计研究院等为代表的单位在铜铅锌复杂多金属矿选矿技术方面也有了一些探索性的研究。
然而,目前仍然需要进一步的研究来解决一些重要的问题,例如一些矿物粒度细、难选等的矿石仍然无法进行有效的投资,这也是矿业行业面临的难题之一。
1.3 研究目的及研究内容本文旨在通过对一种铜铅锌复杂多金属矿进行选矿试验研究,探索一种高效、低成本、节能环保的铜铅锌复杂多金属矿选矿工艺,同时深入分析试验结果,提出进一步完善该工艺的方案,为该类选矿技术的研究提供新的思路和方法。
铜铅锌多金属矿的选矿工艺优化研究摘要:铜铅锌多金属矿是一种重要的矿产资源,在国民经济发展和工业生产中具有重要的地位。
然而,由于其矿石成分复杂多样,选矿工艺的优化对提高矿石的加工回收率和产品质量至关重要。
基于此,本文章对铜铅锌多金属矿的选矿工艺优化进行探讨,以供参考。
关键词:铜铅锌多金属矿;选矿工艺;优化方法Study on beneficiation process optimization of copper-lead-zinc polymetallic oreLengXiao-yanYunnan Diqing Nonferrous Metals Co., LTD., Diqing Tibetan Autonomous Prefecture, Yunnan Province 674400, ChinaAbstract: Copper-lead-zinc polymetallic ore is an important mineral resource, which plays an important role in the development of national economy and industrial production. However, due to the complex and perse composition of its ore, the optimization of beneficiation process is very important to improve the recovery rate and product quality of the ore. Based on this, this paper discusses the beneficiation process optimization of copper-lead-zinc polymetallic ore for reference.Key words: copper-lead-zinc polymetallic ore; Beneficiation process; Optimization method引言铜铅锌多金属矿是一种重要的矿产资源,具有广泛的应用价值。
难选铜锌多金属硫化矿浮选工艺研究我国某铜锌多金属硫化矿,矿体以铜、锌、硫为主,伴生有铜、金、银等。
投产以来,由于原矿含铜品位高,锌矿物里含乳浊状黄铜矿,致使锌的回收指标波动较大,锌精矿含铜超标,锌回收率低。
研究的目的,确实是为了完善工艺流程,提高铜锌分离效率,提高有效金属的回收指标,使锌精矿能够以合格品产出。
考虑到原矿中银的含量较高,达到近80g/t,其工业价值不容轻忽,为了降低硫精矿中银的含量,使之进入到铜、锌精矿产品中,从而减少银的损失,实验方案采纳优先浮铜,锌硫混浮,混合精矿再磨分选的工艺流程。
通过大量的条件实验,找到了铜、锌、硫的可浮性规律,确信了处置该矿相适宜的工艺参数和药剂制度,经闭路实验验证,取得了中意的分选指标。
一、工艺矿物学研究(一)多元素分析及矿物相对含量矿石的多元素分析结果见表1,矿物相对含量见表2。
表1 原矿多元素分析结果 %表2 矿物相对含量 %(二)铜、锌的物相分析铜、锌的物相分析结果见表3、表4。
表3 铜的化学物相分析结果 %表4 锌的化学物相分析结果 %(三)要紧矿物的工艺特点矿体为复杂的多金属硫化矿,要紧矿物的工艺特点如下:黄铜矿:要紧的含铜矿物,含铜量占总铜的80%。
黄铜矿呈不规那么粒状集合体和黄铁矿、白铁矿、闪锌矿、方铅矿紧密嵌生组成致密块状体,或呈不规那么颗粒嵌生在白云石、石英等脉石矿物中。
黄铜矿沿破碎的黄铁矿颗粒裂隙充填成网格状结构,脉宽~0.008mm,较难解离。
有少量黄铜矿发生次生转变,生成辉铜矿、蓝辉铜矿、斑铜矿和铜蓝等充填在黄铁矿颗粒间隙或裂隙中。
黄铜矿的自然粒度范围宽广,但要紧集中在1~0.037mm级别中,0.074mm以下颗粒要紧呈乳浊状和短绒状被包于闪锌矿中。
闪锌矿:要紧的含锌矿物,其含锌量占总锌的80%以上。
闪锌矿在各类矿石中要紧呈不规那么粒状集合体嵌布在黄铁矿、炭酸盐矿物和石英脉中,与黄铜矿、方铅矿紧密嵌生,少量呈自形、半自形晶颗粒嵌布在脉石矿物中。
某难选铜铅锌多金属硫铁矿选矿试验孙康;钱有军【摘要】以某铜铅锌复杂难选多金属硫铁矿为研究对象,在对该矿石工艺矿物学研究的基础上,进行了大量的探索试验研究.试验结果表明:采用铜、铅、锌、硫依次优先浮选,锌精选时采用浮—磁联合工艺流程,在原矿含铜为0.18%、含铅为0.27%、含锌为1.45%、含硫为14.09%的情况下,闭路试验可获得含铜10.68%、铜回收率为41.65%的铜精矿,含铅42.88%、铅回收率为80.04%的铅精矿,含锌42.04%、锌回收率为84.11%的锌精矿,含硫40.21%、硫回收率为62.64%的硫精矿,实现了该多金属硫铁矿的综合利用.【期刊名称】《现代矿业》【年(卷),期】2018(034)009【总页数】5页(P6-10)【关键词】铜铅锌多金属硫铁矿;优先浮选;浮—磁联合工艺【作者】孙康;钱有军【作者单位】西藏玉龙铜业股份有限公司;中钢集团安徽天源科技股份有限公司【正文语种】中文我国有色矿产资源丰富,但近年随着矿山的过度开采,矿石品位逐年降低,矿石性质也越来越复杂,难选多金属矿石所占比例越来越大,如何实现难选多金属矿石的综合利用是目前选矿领域的难点之一[1-2]。
以某铜铅锌复杂难选多金属硫铁矿为研究对象进行了选矿工艺试验研究,确定了适合该矿石分选的工艺流程及药剂制度,实现了对该难选多金属矿的综合利用,并获得了满意的试验指标。
1 矿石性质某铜铅锌复杂难选多金属硫铁矿的主要有价矿物分别为铜、铅、硫、铁等,矿石中主要金属矿物为黄铜矿、方铅矿、闪锌矿、铁闪锌矿、磁黄铁矿、黄铁矿、磁铁矿等;石英、方解石、辉石等为脉石的主要组成部分。
矿石中矿物赋存形式复杂,铜矿物以黄铜矿为主,铅矿物以方铅矿为主,锌矿物主要为闪锌矿和铁闪锌矿,硫铁矿物主要为黄铁矿、磁黄铁矿和少量磁铁矿。
原矿化学多元素分析结果见表1。
表1 原矿化学多元素分析结果 %元素CuPbZnSFe含量0.180.271.4514.0922.05元素SiO2MgONa2OAl2O3CaO含量27.207.530.0450.567.062 选矿试验研究该矿石含硫、铁高,但铜、铅、锌含量较低,并且富含较多的磁黄铁矿、铁闪锌矿,很大程度影响了铜铅锌硫精矿产品的品位。
某复杂铜铅锌多金属矿选矿试验黄建芬【摘要】针对某复杂铜铅锌多金属矿的性质特点,采用弱磁选脱硫—铜铅混浮—混合精矿铜铅分离—混浮尾矿选锌的原则流程对该矿石进行选矿试验研究.在矿石磨矿细度为-0.074 mm占90%的情况下,采用1次弱磁选选硫、1粗2精2扫铜铅混浮、1粗2精1扫铜铅分离、1粗3精2扫选锌、中矿顺序返回流程处理该矿石,最终获得了铜品位为24.79%、铜回收率为55.78%的铜精矿,铅品位为51.34%、铅回收率为83.55%的铅精矿,锌品位为45.63%、锌回收率为62.71%的锌精矿,硫品位为35.12%、硫回收率为80.08%的硫精矿.铜精矿含银229.53g/t,铅精矿含银196.20g/t,铜、铅精矿中银的总回收率为50.29%.%According to the characteristics of Copper-Lead-Zinc Multi-Metal Minerals, beneficiation tests is made by adopting the principle flow-sheet of desuphurization magnetic separation-copper-lead mixed beneficiation-copper-lead separation from rough mixed concentrate-zinc concentration from mixed tailings. Under the grinding fineness of -0.074 mm 90% , the final copper concentrate with Cu grade of 24.79% and recovery of 55.78% , lead concentrate with Pb grade of 51. 34% and recovery of 83.55 % , zinc concentrate with Zn grade of 45. 63 % and recovery of 62. 71 % , Sulfur concentrate with S grade of 35. 12% and the recovery of 80.08% , were obtained respectively through the process of sulfur concentration by one low intensity magnetic separation, copper-lead mixed flotation by one-roughing, two-cleaning and two-scavenging, copper-lead separation by one-roughing, two-cleaning and one-scavenging, zinc concentration byone-roughing, three-cleaning and two-scavenging, and middles back to the flow sheet in order. Copper concentrate contains silver of 229. 53 g/t, and lead concentrate contains silver of 196. 20 g/t. Total silver recovery from copper and lead concentrates reached 50. 29%.【期刊名称】《金属矿山》【年(卷),期】2012(000)011【总页数】5页(P76-79,162)【关键词】铜铅锌多金属矿;脱硫磁选;铜铅混合浮选;铜铅分离;锌浮选;Tc-1;T-101【作者】黄建芬【作者单位】西北矿冶研究院【正文语种】中文某铜铅锌多金属硫化矿共生关系密切,铜品位较低,锌矿物主要为铁闪锌矿,磁黄铁矿含量高达38%,属典型的复杂多金属硫化矿。
矿山建筑M ine building探究铜铅锌多金属矿的选矿工艺常 征,陈长宝(西藏华泰龙矿业开发有限公司,西藏 拉萨 850200)摘 要:矿产资源的选矿作业,是矿产资源在投入市场以前必须完成的加工处理步骤,运用选矿作业能够促使矿产资源去除杂质、有用矿物富集。
本文在开展我国已探明储备的铜铅锌多金属矿的选矿工艺设计时,首先明确了多金属矿对象的采取和加工技术,并结合以往的选矿经验,合理利用浮选工艺流程,完成选矿工艺的实际操作,从而有效地实现了选矿的准确性提升。
关键词:铜铅锌多金属矿;矿产资源;选矿工艺;浮选工艺中图分类号:TD95 文献标识码:A 文章编号:11-5004(2018)06-0042-2选矿工艺的实现要求选矿人员能够依据不同矿石资源所含有的不同的化学性质以及物理性质,对其进行细致分类,并通过碎磨方式,将矿石中有用矿物充分解离,进入到选别流程当中。
完成选矿的矿石资源,使其内部的矿物有用组分达到富集效果,并广泛应用于工业生产的能源消耗当中,从而实现矿石资源的经济价值。
相较于传统的选矿工艺,现阶段选矿工艺为了满足广泛的工业需求,已经有了长足的进步,在选矿精准度、选矿效率方面提升明显。
1铜铅锌多金属矿的矿样制备与试验1.1 铜铅锌多金属矿的矿样制备本文所开展选矿工艺研究的矿石资源来源于某矿区,按技术规范要求,选取代表性矿样50kg,用于试验。
矿样采用三段一闭路碎矿流程对矿样进行破碎,矿样最终通过3mm筛子形成闭路,筛下产品为试验原材料。
将筛下产品进行混匀缩分,最终形成应用于不同试验用途的矿样[1]。
对矿样进行原矿鉴定、化验分析以,其他矿样备用浮选工艺试验。
1.2 试验设备选择为了能够提升选矿工艺的精准性,本文在开展浮选试验之前,首先针对多金属矿的选矿特点,选择了相应的专门实验设备。
其中用于矿样干燥的干燥箱设备选用为ZK型真空干燥箱,而磨矿所采用的球磨机则选用XMQ型锥形球磨机。
此外,电子秤、挂槽以及单槽浮选机等,均为技术先进的仪器设备。
铜铅锌多金属硫化矿浮选分离研究探析本文首先介绍了铜铅锌等金属的性质、作用和资源概况,并阐述了铜铅锌多金属硫化矿分离难的原因,然后重点分析了目前我国在开采铜铅锌多金属硫化矿中常用技术之一的“浮选分离”技术,对其概念、特点、工艺流程和作用进行了具体说明,期待能为矿产开发人员提供一点微不足道的借鉴方法。
标签:铜铅锌多金属硫化矿;浮选分离一、引言众所周知,金属矿产资源是一种不可再生的资源,我国虽然地大物博,矿产资源较为丰富,但是我国矿产资源有先天的缺陷或者说特性,比如品位低、有用矿物嵌布粒度细以及矿物共生复杂等,这就使得在开采矿产时,需要经过很多道工艺和流程,结合先进技术对矿产的各种金属元素进行分离,极其费时费力。
经验和历史都证明,矿物浮选分离技术是先进的选矿方法之一,在处理低品位和复杂难选的矿产时具有其他技术和方法不可比拟的优势。
二、铜铅锌多金属硫化矿的特点铜铅锌多金属硫化矿大多形成于热液型或卡矽岩型矿床中,砂卡岩型矿床矿石以中等品位为主,热液型矿床矿石的品位较低,但热液型矿床工业意义更大,绝大多数的铜铅锌多金属硫化矿石均开釆自深成热液型及中、低温热液型矿床。
该类矿石的主要铜矿物有黄铜矿、斑铜矿、辉铜矿,铅矿物主要为方铅矿,锌矿物主要为闪锌矿、铁闪锌矿,主要的铁矿物为黄铁矿、磁黄铁矿,矿石中还可能含有部分氧化矿物如孔雀石、蓝铜矿、白铅矿等。
铜铅锌多金属硫化矿除含铜、铅、锌等金属元素外,还常伴生镉、铟、金、银,有时矿石还含有硒、钽等稀散元素。
因此,对该类矿石进行综合回收具有巨大的经济价值。
三、铜铅锌多金属硫化矿浮选分离难的原因铜铅锌多金属硫化矿的矿物组成通常较为复杂,难以分离,其原因主要有几点:(1)高温热液型的矿石中,铜矿物往往呈細粒或微细粒浸染状态存在于闪锌矿中。
这矿石中有用矿物致密共生,结晶粒度非常细小,导致三种矿物难以单体解离,分离困难。
即使通过磨矿使三者单体解离,但矿物粒度过细,浮游速度变慢,同时矿粒的比表面积增大,使铜矿物等颗粒的可溶性增加,矿浆中难免离子浓度增大,导致分离效果变差。
西北某复杂铜铅锌银多金属矿选矿工艺研究张雨田;宋翔宇;李荣改;周新民;徐靖【摘要】According to the characteristics of a Cu-Pb-Zn-Ag polymetallic sulfide ore from Northwest China, such as the close paragenetic relationship of minerals and the fine dissemination of copper, lead andzinc minerals, reagents with better selectivity, such as copper collector, YK1 -11, and galena depressant, YK3 -09, were chosen, a Cu-Pb-Zn selective flotation flowsheet was adopted and the Cu/Pb/Zn separation was effectively actualized. A copper concentrate with a copper grade of 17. 12% and a silver content of 4753 g/t can be obtained, while the recovery of copper and silver reached 61. 16% and 83.99% , respectively. Meanwhile, a lead-zinc bulk concentrate containing 25. 19% of lead and 28.5% of zinc can be prepared with recovery of lead and zinc reaching 43. 11% and 33. 1% , respectively. Then, a lead concentrate with a lead grade and recoveryof 48. 11% and 27% , respectively, and a zinc concentrate with a zinc grade and recovery of 43.26% and 43.27% , respectively, can be reclaimed. This study provides a new approach for the exploitation and utilization of Cu-Pb-Zn ore resources.%针对西北某铜铅锌银多金属硫化矿共生关系密切,且铜铅锌矿物嵌布粒度极细的特点,使用选择性较强的铜捕收剂YK1-11和方铅矿抑制剂YK3-09等浮选药剂,采用优先浮选工艺流程,成功实现了铜铅锌的分选,获得铜精矿含铜17.12%、含银4753g/t、铜回收率61.16%、银总回收率83.99%,铅锌混合精矿含铅25.19%、含锌28.5%、铅回收率43.11%、锌回收率33.1%,铅精矿含铅48.11%、铅回收率27%,锌精矿含锌43.26%、锌回收率43.27%的指标.为类似复杂铜铅锌多金属矿的开发与利用提供了新的思路.【期刊名称】《矿冶工程》【年(卷),期】2011(031)003【总页数】4页(P66-69)【关键词】浮选;多金属硫化矿;铅锌矿;优先浮选【作者】张雨田;宋翔宇;李荣改;周新民;徐靖【作者单位】河南省岩石矿物测试中心,河南郑州450012;河南省金属矿产成矿地质过程与资源利用重点实验室,河南郑州450012;河南省岩石矿物测试中心,河南郑州450012;河南省金属矿产成矿地质过程与资源利用重点实验室,河南郑州450012;河南省岩石矿物测试中心,河南郑州450012;河南省金属矿产成矿地质过程与资源利用重点实验室,河南郑州450012;河南省岩石矿物测试中心,河南郑州450012;河南省金属矿产成矿地质过程与资源利用重点实验室,河南郑州450012;河南省岩石矿物测试中心,河南郑州450012;河南省金属矿产成矿地质过程与资源利用重点实验室,河南郑州450012【正文语种】中文【中图分类】TD923铜铅锌复杂多金属矿的分选一直是选矿工作者面临的技术难题。
铜铅锌银多金属矿石选矿工艺研究赵元来发布时间:2021-10-13T07:14:32.172Z 来源:《防护工程》2021年18期作者:赵元来[导读] 目前,世界各地加工的铜锌矿石成分越来越复杂,矿物间的紧密共生和复杂镶嵌已成为重金属研究中最困难的问题之一。
这些矿石在德国和国外主要通过浮选处理。
新疆天地源矿业工程技术有限公司新疆乌鲁木齐 830000摘要:根据矿石性质进行了铜、铅、锌多金属硫化物富集试验,铜浓度为23.37%,铜浓度为63.99%,铅浓度为71.68%,铅浓度为90.34%,铅浓度为1189/T,铜浓度为63.99%,锌含量为63.75%,锌含量为38%和38%。
关键词:铜铅锌;金属矿石;选矿;工艺前言:目前,世界各地加工的铜锌矿石成分越来越复杂,矿物间的紧密共生和复杂镶嵌已成为重金属研究中最困难的问题之一。
这些矿石在德国和国外主要通过浮选处理。
青海省铜与铅共生关系密切,锌、银多金属硫化矿具有铜、铅、锌氧化程度不同的特点,难以分离。
根据矿石性质,成功地实现了铜、铅、锌的分离过程,取得了满意的浮选分离指标。
小铁山是我国主要的铜、铅、锌矿床之一。
矿石中含有许多有价值的元素,如铜、铅、锌、硫、金和银。
“银”选矿厂甲基进料系统投运以来,在浮选过程中,经过多年的生产试验、研究和实践,硫酸盐和硫化钠的分离成为铜精矿,技术进步指标不断提高,铅和锌的指标接近或达到解释值,但铜的指标很低:铜、铅和锌的回收率1998年,金和银分别占34.99%、74.01%和88.28%,而且自1999年以来,选矿企业通过多年的科研生产实践,建立了甲基化生产支撑体系,对工艺条件进行了有效改造和改进,取得了明显效果。
支持系统得到了显著改进,尤其是铜回收率指数的快速增长为公司带来了可观的经济效益。
2003年,铜、铅、锌、金和银的实际回收率分别为60%、80.58%、91.16%、91.01%和82.90%。
实际铜回收率是历史上最好的水平1 矿石性质该矿含有多种矿物,主要有磷灰石、铅、黄铁矿、黄铜矿、铜蓝等。