盐雾试验测试报告)彩锌四通
- 格式:doc
- 大小:585.50 KB
- 文档页数:3
ZHEJIANG PUWONTER MACHINERY CO.,LTD
TEST REPORT(测试报告)
WI-51-010A Product Name(产品名称): SP8558-007 DA TE(日期):2009.10.7-2009.10.11
Test Conducted(测试规范): Salt Spray(Fog) Test (ASTM B 117-03A , ASTM D 610-01)(盐雾试验)
Number Of Test Samples(测试样品的数量): 2 PCS
Salt Solution(盐的溶液): 5% SODIUM CHLORIDE DESSOLVE IN 95% DISTILL WATER(PH=6.5 TO 7.2)
Test Duration(测试持续时间): 96 HOURS(96小时)
Test Machine(测试机器): SALT SPRAY TESTER(HG67)(盐雾试验机)
Arrangement Angle(放置的角度): A T 15-30°FROM VERTICAL
Test Temperature(测试温度): 35+1.1/ -1.7°C
V olume of collected solution(采集溶液的容积): 1.0~2.0ML/80CM²/HOUR
Saturator Tower Temperature(温度饱和器): 47±1°C
Test Results
sample Description Sample NO Rating(Observation) Type of deterioration 样品描述样品编号等级级别(观察) 腐蚀的类型
72 huors-No corrosion
NO1,NO2 10 S
observed
Observation Rating(观察的等级级别):
0=>50.0% Rust 1=33.3-50.0% Rust 2=16.0-33.3% Rust
3=10.0-16.0% Rust 4=3.0-10.0% Rust 5=1.0-3.0% Rust
6=0.3-1.0% Rust 7=0.1-0.3% Rust 8=0.03-0.1% Rust
9=0.01-0.03% Rust 10=<=0.01% Rust
Type of deterioration(腐蚀类型)
S:Spot Rusting(点腐蚀)
G:General Rusting(大面积腐蚀)
P:Pinpoint Rusting(细微腐蚀)
H:Hybird Rusting(混合腐蚀)
WI-51-010A Product Name(产品名称): TCHDA-1 PUSH-OM-1DATE(日期):09-04-20
Remark:-The photo is undersurface.(备注:如下照片)
Before test
Approved(审核):NEO Inspector(检验员):Mike Gao